Essentials of GB/T 228.1 Tensile Testing: Specimen, Rate Control and Yield Determination

Gauge length L₀=5.65√S₀, stress rate 2-60 MPa/s before yield; read ReH/ReL for sharp yield, Rp0.2 otherwise.

华旋光电技术部
Essentials of GB/T 228.1 Tensile Testing: Specimen, Rate Control and Yield Determination

Specimen and gauge length

GB/T 228.1, corresponding to ISO 6892-1, defines proportional specimens with original gauge length L₀=k√S₀, where k is 5.65 for short and 11.3 for long specimens; a 10 mm round bar with S₀=78.5 mm² gets L₀=50 mm. Mark the gauge with fine scribe lines or a dot punch; notch effects from rough marking lower the measured elongation. The transition radii between grip and parallel sections must be machined properly. Fracture outside the gauge length near the grips invalidates the result unless elongation still meets requirements and both parties accept it.

Rate control

Rates split into two stages: before yield, control stress rate within 2-60 MPa/s in the elastic range, commonly 6-20 MPa/s; after yield, switch to strain-rate control, with method A specifying 0.00025 to 0.0025 s⁻¹. Running too fast inflates yield strength by 10-30 MPa, the most common cause of interlaboratory disagreement. Older machines without closed-loop strain control may approximate it by crosshead speed, but the method must be stated in the report.

Yield determination

Materials with a clear yield plateau, such as low-carbon steels, give upper and lower yield strengths ReH and ReL: ReH is the maximum force before the first drop, ReL the minimum on the plateau ignoring initial transients. Materials without a distinct yield, such as aluminium alloys and quenched-tempered steels, require the 0.2 percent proof strength Rp0.2: draw a line parallel to the elastic slope offset by 0.2 percent of gauge length, and the intersection gives Rp0.2. An extensometer is mandatory here; crosshead displacement is no substitute.

Validity of results

Elongation after fracture A and reduction of area Z are measured on the reassembled broken specimen, minimizing alignment error. Test temperature is 23±5 °C, or 23±2 °C for referee tests. At least two valid specimens per group; round strengths to 1 MPa and elongation to 0.5 percent per GB/T 8170. Reports must state the rate-control method and extensometer gauge length — auditors will return reports missing either item.